If you specify conductors for aerospace, defense or outdoor cable, you already know that a material's day-one numbers are the easy part. What you need to know is how it behaves after a qualification-style environmental exposure. We put Galvorn® yarns, bare and ETFE-insulated, through accelerated aging testing at an independent lab: 500 hours of xenon-arc UV weathering, 500 hours of cyclic salt fog, and a 1,000-hour life test at 150 °C followed by ten thermal shock cycles from -65 °C to 150 °C. We then measured break force and resistance before and after each exposure, with para-aramid and ultra-high-molecular-weight polyethylene (UHMWPE) fibers alongside as strength benchmarks.
The headline result is for the insulated yarn. Across all three exposures, ETFE-insulated Galvorn® yarn kept 94 to 97% of its specific conductivity and 97 to 98% of its break force, in a single run per exposure. UV was the hardest of the three, and the insulated yarn came through it with about 97% of its break force and 96% of its conductivity. Below we walk through what each exposure did, what the insulation changed, and what we haven't tested yet.
What does accelerated aging testing tell you about a conductor?
Accelerated aging testing exposes a material to UV light, salt spray or temperature cycling at a higher intensity than it would see in service, so years of wear show up in weeks. For a conductor, you compare break force and electrical resistance before and after, and the share that remains is the margin you keep. In this round of accelerated aging testing, ETFE-insulated Galvorn® yarn, an advanced carbon conductor, kept 94 to 97% of its specific conductivity through UV, salt fog and thermal cycling, in a single run per exposure.
Three exposures, one lab, one measurement method
The samples were aged at an independent accelerated weathering lab and measured by DexMat before and after exposure, so each result compares lengths of the same yarn before and after aging. Each condition was run once, on a single 5 m length of each material, which gave several break force, resistance and linear density measurements per sample. The exposures were:
- UV: 500 hours of xenon-arc weathering (ASTM G155 cycle 1, 0.35 W/m²·nm at 340 nm).
- Salt fog: 500 hours of cyclic salt fog (5% NaCl at 35 °C, per ASTM B117).
- Thermal cycling: a 1,000-hour life test at 150 °C per MIL-DTL-32630, followed by MIL-STD-202 Method 107 thermal shock (Condition F).
The Galvorn® samples were bare Galvorn® 800 and Galvorn® 1000 yarns in four sizes from about 150 to 500 microns, in as-spun, baked and annealed conditions, plus one Galvorn® 800 Twisted Yarn at 400 microns with an extruded ETFE insulation. The aramid and UHMWPE fibers ran alongside as mechanical benchmarks; neither conducts, so they appear only in the strength results.
Sunlight is the enemy of every fiber, and insulation is the answer
UV is the exposure most likely to end up in a harness specification for anything that lives outdoors or near a window, and it was the harshest condition in this test for every material. Bare Galvorn® yarns kept 55 to 84% of their break force after 500 hours of xenon arc. The aramid fiber lost more, falling to about 40% of its break force; the UHMWPE fiber kept about 70%. Bare as-spun Galvorn yarns kept 58 to 67% of their specific conductivity.
Put a standard ETFE insulation over the yarn and the picture changes. ETFE-insulated Galvorn® yarn kept about 97% of its break force and about 96% of its specific conductivity after the same 500 hours of UV. The insulation takes the UV and the conductor underneath does its job.
| Sample | Break force, N (before → after) | Break force (% of original) | Specific conductivity (% of original) |
|---|---|---|---|
| Galvorn 800 yarn, 400 µm, bare | 44.8 → 32.9 | 73 | 58 |
| Galvorn 800 yarn, 500 µm, bare | 101 → 61.2 | 61 | 58 |
| Galvorn 1000 yarn, 150 µm, bare | 21.4 → 17.9 | 83 | 64 |
| Galvorn 1000 yarn, 500 µm, bare | 233 → 134 | 57 | 67 |
| Galvorn 800 Twisted Yarn, 400 µm, ETFE-insulated | 60.2 → 58.5 | 97 | 96 |
| Aramid fiber | 133 → 53.2 | 40 | n/a (not conductive) |
| UHMWPE fiber | 67.4 → 46.8 | 69 | n/a (not conductive) |
Salt fog leaves strength alone and the insulation holds conductivity
Salt fog matters for anything on a ship, a coastal site or an aircraft that sees sea air. Bare Galvorn® yarns kept at least 90% of their original break force after 500 hours, with no measurable loss in three of the four as-spun yarns, so corrosion did not take strength from the carbon itself. Conductivity moved more: as-spun bare yarns kept about 77 to 83% of their specific conductivity. ETFE-insulated Galvorn® yarn kept about 98% of its break force and about 97% of its specific conductivity, with resistance per meter essentially unchanged.
| Sample | Break force, N (before → after) | Break force (% of original) | Specific conductivity (% of original) |
|---|---|---|---|
| Galvorn 800 yarn, 400 µm, bare | 44.8 → 45.5 | No measurable loss | 79 |
| Galvorn 800 yarn, 500 µm, bare | 101 → 108 | No measurable loss | 80 |
| Galvorn 1000 yarn, 150 µm, bare | 21.4 → 22.2 | No measurable loss | 77 |
| Galvorn 1000 yarn, 500 µm, bare | 233 → 210 | 90 | 83 |
| Galvorn 800 Twisted Yarn, 400 µm, ETFE-insulated | 60.2 → 59.0 | 98 | 97 |
| Aramid fiber | 133 → 135 | No measurable loss | n/a (not conductive) |
| UHMWPE fiber | 67.4 → 67.7 | 100 | n/a (not conductive) |
Strength holds through 1,000 hours at 150 °C and shock cycling
Thermal cycling is the exposure engine bays and avionics bays care about. Bare Galvorn® yarns kept at least 93% of their original break force after the 1,000-hour life test at 150 °C and ten shock cycles from -65 °C to 150 °C. As-spun bare yarns kept about 70 to 86% of their specific conductivity. ETFE-insulated Galvorn® yarn kept about 98% of its break force and about 94% of its specific conductivity, with resistance per meter up about 14%. The insulated yarn is the one sample in the set that came through all three exposures above 90% on both strength and conductivity.
| Sample | Break force, N (before → after) | Break force (% of original) | Specific conductivity (% of original) |
|---|---|---|---|
| Galvorn 800 yarn, 400 µm, bare | 44.8 → 41.5 | 93 | 70 |
| Galvorn 800 yarn, 500 µm, bare | 101 → 109 | No measurable loss | 75 |
| Galvorn 1000 yarn, 150 µm, bare | 21.4 → 20.5 | 96 | 78 |
| Galvorn 1000 yarn, 500 µm, bare | 233 → 223 | 96 | 86 |
| Galvorn 800 Twisted Yarn, 400 µm, ETFE-insulated | 60.2 → 59.2 | 98 | 94 |
| Aramid fiber | 133 → 113 | 85 | n/a (not conductive) |
| UHMWPE fiber | 67.4 → n/a | exceeds rated temperature | n/a (not conductive) |
Bare where it's protected, insulated where it isn't
Two practical conclusions fall out of this. First, bare Galvorn® yarn keeps its strength through salt fog and thermal cycling and keeps 55 to 84% of it through UV, so it is a reasonable choice inside a composite, under an overbraid, or anywhere else the environment can't reach it directly. Second, for an exposed conductor the standard answer works: a conventional extruded insulation closes the gap, and an insulated Galvorn® conductor holds its properties through the full exposure set. Galvorn® yarn has already been run through cable manufacturers' extrusion lines with ETFE and FEP insulation, so this is a construction a cable shop can build today rather than a lab-only sample.
This is our first round of accelerated aging on these constructions, and we'll keep adding exposures and products. Two things you'll want to know were outside this round: thermal aging beyond 1,000 hours and flex life under load after exposure.
Frequently asked questions
If you're evaluating Galvorn® for a harness or cable that has to pass environmental qualification, contact DexMat's engineering team. We can share the test conditions in detail and talk through which construction fits your exposure set.